Melting points of the elements (data page)

Main article: Melting point

Melting point

Reference Kelvin Celsius Fahrenheit Comments
1 H hydrogen (H2)
use 13.99 K −259.16 Â°C −434.49 Â°F
WEL 14.01 K −259.14 Â°C −434.45 Â°F
CRC −259.16 Â°C
LNG −259.35 Â°C
2 He helium
use 0 K −273.15 Â°C −459.67 Â°F hcp crystal melting to He-II superfluid at 25.00 atm
1.463 K −271.687 Â°C −457.037 Â°F triple point hcp−bcc−He-II at 26.036 atm
1.762 K −271.388 Â°C −456.498 Â°F triple point hcp−bcc−He-II at 29.725 atm
1.772 K −271.378 Â°C −456.480 Â°F triple point hcp−He-II−He-I at 30.016 atm
WEL 0.95 K −272.2 Â°C −458 Â°F
LNG −272.15 Â°C (at 25 atm)
Hoffer et al. 0 K −273.15 Â°C −459.67 Â°F hcp crystal melting to He-II superfluid at 25.00 atm
1.463 K −271.687 Â°C −457.037 Â°F triple point hcp−bcc−He-II at 26.036 atm
1.762 K −271.388 Â°C −456.498 Â°F triple point hcp−bcc−He-II at 29.725 atm
1.772 K −271.378 Â°C −456.480 Â°F triple point hcp−He-II−He-I at 30.016 atm
3 Li lithium
use 453.65 K 180.50 Â°C 356.90 Â°F
WEL 453.69 K 180.54 Â°C 356.97 Â°F
CRC 180.50 Â°C
LNG 180.54 Â°C
4 Be beryllium
use 1560 K 1287 Â°C 2349 Â°F
WEL 1560 K 1287 Â°C 2349 Â°F
CRC 1287 Â°C
LNG 1287 Â°C
5 B boron
use 2349 K 2076 Â°C 3769 Â°F
WEL 2349 K 2076 Â°C 3769 Â°F
CRC 2075 Â°C
LNG 2076 Â°C
6 C carbon (graphite)
use
WEL ? (3800 K) ? (3527 Â°C) ? (6381 Â°F)
CRC tp 4489 Â°C (at 10.3 MPa)
LNG subl. (3915–4020) °C
6 C carbon (diamond)
use
WEL ? (3800 K) ? (3527 Â°C) ? (6381 Â°F)
CRC 4440 Â°C (at 12.4 GPa)
LNG 3500 Â°C (at 63.5 atm)
7 N nitrogen (N2)
use 63.15 K −210.00 Â°C −346.00 Â°F
WEL 63.05 K −210.1 Â°C −346.18 Â°F
CRC −210.00 Â°C
LNG −210.01 Â°C
8 O oxygen (O2)
use 54.36 K −218.79 Â°C −361.82 Â°F
WEL 54.8 K −218.3 Â°C −360.9 Â°F
CRC −218.79 Â°C
LNG −218.4 Â°C
9 F fluorine (F2)
use 53.48 K −219.67 Â°C −363.41 Â°F
WEL 53.53 K −219.62 Â°C −363.32 Â°F
CRC tp −219.67 Â°C
LNG −219.61 Â°C
10 Ne neon
use 24.56 K −248.59 Â°C −415.46 Â°F
WEL 24.56 K −248.59 Â°C −415.46 Â°F
CRC −248.59 Â°C
LNG −248.67 Â°C
11 Na sodium
use 370.944 K 97.794 Â°C 207.9 Â°F
WEL 370.87 K 97.72 Â°C 207.9 Â°F
CRC 97.794 Â°C
LNG 97.82 Â°C
12 Mg magnesium
use 923 K 650 Â°C 1202 Â°F
WEL 923 K 650 Â°C 1202 Â°F
CRC 650 Â°C
LNG 651 Â°C
13 Al aluminium
use 933.47 K 660.32 Â°C 1220.58 Â°F
WEL 933.47 K 660.32 Â°C 1220.58 Â°F
CRC 660.32 Â°C
LNG 660.323 Â°C
freezing point 933.473 K (660.323 Â°C) fixed point on ITS-90
14 Si silicon
use 1687 K 1414 Â°C 2577 Â°F
WEL 1687 K 1414 Â°C 2577 Â°F
CRC 1414 Â°C
LNG 1412 Â°C
15 P phosphorus (white)
use 317.30 K 44.15 Â°C 111.47 Â°F
WEL 317.3 K 44.2 Â°C 111.6 Â°F
CRC 44.15 Â°C
LNG 44.15 Â°C
15 P phosphorus (red)
use 870 K 597 Â°C 1107 Â°F
CRC tp 590 Â°C
LNG 597 Â°C
15 P phosphorus (black)
use 883 K 610 Â°C 1130 Â°F
CRC 610 Â°C
LNG
16 S sulfur (orthorhombic, alpha)
use 368.4 K 95.3 Â°C 203.5 Â°F (trans. to beta)
CRC 95.3 Â°C (trans. to mono)
LNG 94.5 Â°C (trans. to beta)
16 S sulfur (monoclinic, beta, trans. slowly to alpha)
use 388.36 K 115.21 Â°C 239.38 Â°F
WEL 388.36 K 115.21 Â°C 239.38 Â°F
CRC 119.6 Â°C
LNG 115.21 Â°C
16 S sulfur (gamma)
use 380.0 K 106.8 Â°C 224.2 Â°F
LNG 106.8 Â°C
17 Cl chlorine (Cl2)
use 171.6 K −101.5 Â°C −150.7 Â°F
WEL 171.6 K −101.5 Â°C −150.7 Â°F
CRC −101.5 Â°C
LNG −101.5 Â°C
18 Ar argon
use 83.81 K −189.34 Â°C −308.81 Â°F
WEL 83.8 K −189.3 Â°C −308.7 Â°F
CRC −189.34 Â°C
LNG −189.38 Â°C
19 K potassium
use 336.7 K 63.5 Â°C 146.3 Â°F
WEL 336.53 K 63.38 Â°C 146.08 Â°F
CRC 63.5 Â°C
LNG 63.38 Â°C
20 Ca calcium
use 1115 K 842 Â°C 1548 Â°F
WEL 1115 K 842 Â°C 1548 Â°F
CRC 842 Â°C
LNG 842 Â°C
21 Sc scandium
use 1814 K 1541 Â°C 2806 Â°F
WEL 1814 K 1541 Â°C 2806 Â°F
CRC 1541 Â°C
LNG 1541 Â°C
22 Ti titanium (hexagonal)
use 1941 K 1668 Â°C 3034 Â°F
WEL 1941 K 1668 Â°C 3034 Â°F
CRC 1668 Â°C
LNG 1668 Â°C
23 V vanadium
use 2183 K 1910 Â°C 3470 Â°F
WEL 2183 K 1910 Â°C 3470 Â°F
CRC 1910 Â°C
LNG 1917 Â°C
24 Cr chromium
use 2180 K 1907 Â°C 3465 Â°F
WEL 2180 K 1907 Â°C 3465 Â°F
CRC 1907 Â°C
LNG 1907 Â°C
25 Mn manganese
use 1519 K 1246 Â°C 2275 Â°F
WEL 1519 K 1246 Â°C 2275 Â°F
CRC 1246 Â°C
LNG 1244 Â°C (face-centered tetragonal)
26 Fe iron
use 1811 K 1538 Â°C 2800 Â°F
WEL 1811 K 1538 Â°C 2800 Â°F
CRC 1538 Â°C
LNG 1535 Â°C
27 Co cobalt
use 1768 K 1495 Â°C 2723 Â°F
WEL 1768 K 1495 Â°C 2723 Â°F
CRC 1495 Â°C
LNG 1494 Â°C
28 Ni nickel
use 1728 K 1455 Â°C 2651 Â°F
WEL 1728 K 1455 Â°C 2651 Â°F
CRC 1455 Â°C
LNG 1453 Â°C
29 Cu copper
use 1357.77 K 1084.62 Â°C 1984.32 Â°F
WEL 1357.77 K 1084.62 Â°C 1984.32 Â°F
CRC 1084.62 Â°C
LNG 1084.62 Â°C
freezing point 1357.77 K (1084.62 Â°C) fixed point on ITS-90
30 Zn zinc
use 692.68 K 419.53 Â°C 787.15 Â°F
WEL 692.68 K 419.53 Â°C 787.15 Â°F
CRC 419.53 Â°C
LNG 419.527 Â°C
freezing point 692.677 K (419.527 Â°C) fixed point on ITS-90
31 Ga gallium
use 302.9146 K 29.7646 Â°C 85.5763 Â°F
WEL 302.91 K 29.76 Â°C 85.57 Â°F
CRC tp 29.771 Â°C
LNG 29.7646 Â°C
melting point 302.9146 K (29.7646 Â°C) fixed point on ITS-90
32 Ge germanium
use 1211.40 K 938.25 Â°C 1720.85 Â°F
WEL 1211.4 K 938.3 Â°C 1720.9 Â°F
CRC 938.25 Â°C
LNG 937.3 Â°C
33 As arsenic
use 1090 K 817 Â°C 1503 Â°F
WEL 1090 K 817 Â°C 1503 Â°F
CRC tp 817 Â°C (at 3.70 MPa)
LNG 817 Â°C
34 Se selenium (hexagonal, gray)
use 494 K 221 Â°C 430 Â°F
WEL 494 K 221 Â°C 430 Â°F
CRC 220.5 Â°C
LNG 217 Â°C
34 Se selenium (vitreous)
use 453 K 180 Â°C 356 Â°F (trans. to gray)
CRC 180 Â°C (trans. to gray)
35 Br bromine (Br2)
use 265.8 K −7.3 Â°C 19 Â°F
WEL 265.8 K −7.3 Â°C 19 Â°F
CRC −7.2 Â°C
LNG −7.25 Â°C
36 Kr krypton
use 115.78 K −157.37 Â°C −251.27 Â°F
WEL 115.79 K −157.37 Â°C −251.25 Â°F
CRC tp −157.38 Â°C (at 73.2 kPa)
LNG −157.36 Â°C
37 Rb rubidium
use 312.45 K 39.30 Â°C 102.74 Â°F
WEL 312.46 K 39.31 Â°C 102.76 Â°F
CRC 39.30 Â°C
LNG 39.31 Â°C
38 Sr strontium
use 1050 K 777 Â°C 1431 Â°F
WEL 1050 K 777 Â°C 1431 Â°F
CRC 777 Â°C
LNG 757 Â°C
39 Y yttrium
use 1799 K 1526 Â°C 2779 Â°F
WEL 1799 K 1526 Â°C 2779 Â°F
CRC 1522 Â°C
LNG 1522 Â°C
40 Zr zirconium
use 2128 K 1855 Â°C 3371 Â°F
WEL 2128 K 1855 Â°C 3371 Â°F
CRC 1855 Â°C
LNG 1852 Â°C
41 Nb niobium
use 2750 K 2477 Â°C 4491 Â°F
WEL 2750 K 2477 Â°C 4491 Â°F
CRC 2477 Â°C
LNG 2468 Â°C
42 Mo molybdenum
use 2896 K 2623 Â°C 4753 Â°F
WEL 2896 K 2623 Â°C 4753 Â°F
CRC 2623 Â°C
LNG 2622 Â°C
43 Tc technetium (Tc-98 ?)
use 2430 K 2157 Â°C 3915 Â°F
WEL 2430 K 2157 Â°C 3915 Â°F
CRC 2157 Â°C
LNG 2157 Â°C (Tc-98)
44 Ru ruthenium
use 2607 K 2334 Â°C 4233 Â°F
WEL 2607 K 2334 Â°C 4233 Â°F
CRC 2334 Â°C
LNG 2334 Â°C
45 Rh rhodium
use 2237 K 1964 Â°C 3567 Â°F
WEL 2237 K 1964 Â°C 3567 Â°F
CRC 1964 Â°C
LNG 1963 Â°C
46 Pd palladium
use 1828.05 K 1554.9 Â°C 2830.82 Â°F
WEL 1828.05 K 1554.9 Â°C 2830.82 Â°F
CRC 1554.9 Â°C
LNG 1555 Â°C
47 Ag silver
use 1234.93 K 961.78 Â°C 1763.2 Â°F
WEL 1234.93 K 961.78 Â°C 1763.2 Â°F
CRC 961.78 Â°C
LNG 961.78 Â°C
freezing point 1234.93 K (961.78 Â°C) fixed point on ITS-90
48 Cd cadmium
use 594.22 K 321.07 Â°C 609.93 Â°F
WEL 594.22 K 321.07 Â°C 609.93 Â°F
CRC 321.07 Â°C
LNG 321 Â°C
49 In indium
use 429.75 K 156.60 Â°C 313.88 Â°F
WEL 429.75 K 156.6 Â°C 313.88 Â°F
CRC 156.60 Â°C
LNG 156.60 Â°C
freezing point 429.7485 K (156.5985 Â°C) fixed point on ITS-90
50 Sn tin (white)
use 505.08 K 231.93 Â°C 449.47 Â°F
WEL 505.08 K 231.93 Â°C 449.47 Â°F
CRC 231.93 Â°C
LNG 231.928 Â°C
freezing point 505.078 K (231.928 Â°C) fixed point on ITS-90
51 Sb antimony
use 903.78 K 630.63 Â°C 1167.13 Â°F
WEL 903.78 K 630.63 Â°C 1167.13 Â°F
CRC 630.63 Â°C
LNG 630.7 Â°C
52 Te tellurium
use 722.66 K 449.51 Â°C 841.12 Â°F
WEL 722.66 K 449.51 Â°C 841.12 Â°F
CRC 449.51 Â°C
LNG 449.8 Â°C
53 I iodine (I2)
use 386.85 K 113.7 Â°C 236.66 Â°F
WEL 386.85 K 113.7 Â°C 236.66 Â°F
CRC 113.7 Â°C
LNG 113.60 Â°C
54 Xe xenon
use 161.40 K −111.75 Â°C −169.15 Â°F
WEL 161.4 K −111.7 Â°C −169.1 Â°F
CRC tp −111.795 Â°C (at 81.6 kPa)
LNG −111.8 Â°C
55 Cs caesium
use 301.7 K 28.5 Â°C 83.3 Â°F
WEL 301.59 K 28.44 Â°C 83.19 Â°F
CRC 28.5 Â°C
LNG 28.44 Â°C
56 Ba barium
use 1000 K 727 Â°C 1341 Â°F
WEL 1000 K 727 Â°C 1341 Â°F
CRC 727 Â°C
LNG 726.9 Â°C
57 La lanthanum
use 1193 K 920 Â°C 1688 Â°F
WEL 1193 K 920 Â°C 1688 Â°F
CRC 918 Â°C
LNG 920 Â°C
58 Ce cerium
use 1068 K 795 Â°C 1463 Â°F
WEL 1068 K 795 Â°C 1463 Â°F
CRC 798 Â°C
LNG 795 Â°C
59 Pr praseodymium
use 1208 K 935 Â°C 1715 Â°F
WEL 1208 K 935 Â°C 1715 Â°F
CRC 931 Â°C
LNG 935 Â°C
60 Nd neodymium
use 1297 K 1024 Â°C 1875 Â°F
WEL 1297 K 1024 Â°C 1875 Â°F
CRC 1021 Â°C
LNG 1024 Â°C
61 Pm promethium (Pm-147 ?)
use 1315 K 1042 Â°C 1908 Â°F
WEL 1373 K 1100 Â°C 2012 Â°F
CRC 1042 Â°C
LNG 1080 Â°C (Pm-147)
62 Sm samarium
use 1345 K 1072 Â°C 1962 Â°F
WEL 1345 K 1072 Â°C 1962 Â°F
CRC 1074 Â°C
LNG 1074 Â°C
63 Eu europium
use 1099 K 826 Â°C 1519 Â°F
WEL 1099 K 826 Â°C 1519 Â°F
CRC 822 Â°C
LNG 822 Â°C
64 Gd gadolinium
use 1585 K 1312 Â°C 2394 Â°F
WEL 1585 K 1312 Â°C 2394 Â°F
CRC 1313 Â°C
LNG 1312 Â°C
65 Tb terbium
use 1629 K 1356 Â°C 2473 Â°F
WEL 1629 K 1356 Â°C 2473 Â°F
CRC 1356 Â°C
LNG 1356 Â°C
66 Dy dysprosium
use 1680 K 1407 Â°C 2565 Â°F
WEL 1680 K 1407 Â°C 2565 Â°F
CRC 1412 Â°C
LNG 1412 Â°C
67 Ho holmium
use 1734 K 1461 Â°C 2662 Â°F
WEL 1734 K 1461 Â°C 2662 Â°F
CRC 1474 Â°C
LNG 1474 Â°C
68 Er erbium
use 1802 K 1529 Â°C 2784 Â°F
WEL 1770 K 1497 Â°C 2727 Â°F
CRC 1529 Â°C
LNG 1529 Â°C
talk
  • The Gmelin rare earths handbook lists 1522 Â°C and 1550 Â°C as two melting points given in the literature, the most recent reference [Handbook on the chemistry and physics of rare earths, vol.12 (1989)] is given with 1529 Â°C.
  • The World Book encyclopedia from 2002 lists 1529 Â°C.
69 Tm thulium
use 1818 K 1545 Â°C 2813 Â°F
WEL 1818 K 1545 Â°C 2813 Â°F
CRC 1545 Â°C
LNG 1545 Â°C
70 Yb ytterbium
use 1097 K 824 Â°C 1515 Â°F
WEL 1097 K 824 Â°C 1515 Â°F
CRC 819 Â°C
LNG 819 Â°C
71 Lu lutetium
use 1925 K 1652 Â°C 3006 Â°F
WEL 1925 K 1652 Â°C 3006 Â°F
CRC 1663 Â°C
LNG 1663 Â°C
72 Hf hafnium
use 2506 K 2233 Â°C 4051 Â°F
WEL 2506 K 2233 Â°C 4051 Â°F
CRC 2233 Â°C
LNG 2227 Â°C
73 Ta tantalum
use 3290 K 3017 Â°C 5463 Â°F
WEL 3290 K 3017 Â°C 5463 Â°F
CRC 3017 Â°C
LNG 2996 Â°C
74 W tungsten
use 3695 K 3422 Â°C 6192 Â°F
WEL 3695 K 3422 Â°C 6192 Â°F
CRC 3422 Â°C
LNG 3387 Â°C
75 Re rhenium
use 3459 K 3186 Â°C 5767 Â°F
WEL 3459 K 3186 Â°C 5767 Â°F
CRC 3186 Â°C
LNG 3180 Â°C
76 Os osmium
use 3306 K 3033 Â°C 5491 Â°F
WEL 3306 K 3033 Â°C 5491 Â°F
CRC 3033 Â°C
LNG 3045 Â°C
77 Ir iridium
use 2719 K 2446 Â°C 4435 Â°F
WEL 2739 K 2466 Â°C 4471 Â°F
CRC 2446 Â°C
LNG 2447 Â°C
78 Pt platinum
use 2041.4 K 1768.3 Â°C 3214.9 Â°F
WEL 2041.4 K 1768.3 Â°C 3214.9 Â°F
CRC 1768.4 Â°C
LNG 1769 Â°C
79 Au gold
use 1337.33 K 1064.18 Â°C 1947.52 Â°F
WEL 1337.33 K 1064.18 Â°C 1947.52 Â°F
CRC 1064.18 Â°C
LNG 1064.18 Â°C
freezing point 1337.33 K (1064.18 Â°C) fixed point on ITS-90
80 Hg mercury
use 234.32 K −38.83 Â°C −37.89 Â°F
WEL 234.32 K −38.83 Â°C −37.89 Â°F
CRC tp −38.837 Â°C
LNG −38.83 Â°C
81 Tl thallium
use 577 K 304 Â°C 579 Â°F
WEL 577 K 304 Â°C 579 Â°F
CRC 304 Â°C
LNG 303.5 Â°C
82 Pb lead
use 600.61 K 327.46 Â°C 621.43 Â°F
WEL 600.61 K 327.46 Â°C 621.43 Â°F
CRC 327.46 Â°C
LNG 327.43 Â°C
83 Bi bismuth
use 544.7 K 271.5 Â°C 520.7 Â°F
WEL 544.4 K 271.3 Â°C 520.3 Â°F
CRC 271.40 Â°C
LNG 271.5 Â°C
84 Po polonium
use 527 K 254 Â°C 489 Â°F
WEL 527 K 254 Â°C 489 Â°F
CRC 254 Â°C
LNG 254 Â°C
85 At astatine
use 575 K 302 Â°C 576 Â°F
WEL 575 K 302 Â°C 576 Â°F
CRC 302 Â°C
LNG 302 Â°C
86 Rn radon
use 202 K −71 Â°C −96 Â°F
WEL 202 K −71 Â°C −96 Â°F
CRC −71 Â°C
LNG −71 Â°C
87 Fr francium
use 300 K 27 Â°C 80 Â°F
CRC 27 Â°C
88 Ra radium
use 973 K 700 Â°C 1292 Â°F
WEL 973 K 700 Â°C 1292 Â°F
CRC 700 Â°C
LNG 700.1 Â°C
89 Ac actinium (Ac-227 ?)
use circa 1323 K circa 1050 Â°C circa 1922 Â°F
WEL 1323 K 1050 Â°C 1922 Â°F
CRC 1051 Â°C
LNG 1050(50) °C (Ac-227)
90 Th thorium
use 2115 K 1842 Â°C 3348 Â°F
WEL 2115 K 1842 Â°C 3348 Â°F
CRC 1750 Â°C
LNG 1750 Â°C
91 Pa protactinium
use 1841 K 1568 Â°C 2854 Â°F
WEL 1841 K 1568 Â°C 2854 Â°F
CRC 1572 Â°C
92 U uranium
use 1405.3 K 1132.2 Â°C 2070 Â°F
WEL 1405.3 K 1132.2 Â°C 2070 Â°F
CRC 1135 Â°C
LNG 1135 Â°C
93 Np neptunium
use 917 K 644 Â°C 1191 Â°F
WEL 910 K 637 Â°C 1179 Â°F
CRC 644 Â°C
LNG 644 Â°C
94 Pu plutonium
use 912.5 K 639.4 Â°C 1182.9 Â°F
WEL 912.5 K 639.4 Â°C 1182.9 Â°F
CRC 640 Â°C
LNG 639.5 Â°C
95 Am americium
use 1449 K 1176 Â°C 2149 Â°F
WEL 1449 K 1176 Â°C 2149 Â°F
CRC 1176 Â°C
LNG 1176 Â°C
96 Cm curium (Cm-244 ?)
use 1613 K 1340 Â°C 2444 Â°F
WEL 1613 K 1340 Â°C 2444 Â°F
CRC 1345 Â°C
LNG 1340 Â°C (Cm-244)
97 Bk berkelium (alpha)
use 1323 K 1050 Â°C 1922 Â°F
CRC 1050 Â°C
LNG 1050 Â°C
97 Bk berkelium (beta)
use 1259 K 986 Â°C 1807 Â°F
WEL 1259 K 986 Â°C 1807 Â°F
CRC 986 Â°C
LNG 986 Â°C
98 Cf californium (Cf-252 ?)
use 1173 K 900 Â°C 1652 Â°F
WEL 1173 K 900 Â°C 1652 Â°F
CRC 900 Â°C
LNG 900 Â°C (Cf-252)
99 Es einsteinium
use 1133 K 860 Â°C 1580 Â°F
WEL 1133 K 860 Â°C 1580 Â°F
CRC 860 Â°C
LNG 860 Â°C
100 Fm fermium (Fm-257 ?)
use 1800 K 1527 Â°C 2781 Â°F
WEL 1800 K 1527 Â°C 2781 Â°F
CRC 1527 Â°C
LNG 1527 Â°C (Fm-257)
101 Md mendelevium
use 1100 K 827 Â°C 1521 Â°F
WEL 1100 K 827 Â°C 1521 Â°F
CRC 827 Â°C
102 No nobelium
use 1100 K 827 Â°C 1521 Â°F
WEL 1100 K 827 Â°C 1521 Â°F
CRC 827 Â°C
103 Lr lawrencium
use 1900 K 1627 Â°C 2961 Â°F
WEL 1900 K 1627 Â°C 2961 Â°F
CRC 1627 Â°C
LNG 1627 Â°C

Notes

References

WEL

As quoted at http://www.webelements.com/ from these sources:

CRC

LNG

As quoted from:

Hoffer et al.

See also

This article is issued from Wikipedia - version of the Tuesday, March 15, 2016. The text is available under the Creative Commons Attribution/Share Alike but additional terms may apply for the media files.